Miller CS410A Instrukcja obsługi - Strona 16

Przeglądaj online lub pobierz pdf Instrukcja obsługi dla Latarka Miller CS410A. Miller CS410A 20 stron.

Miller CS410A Instrukcja obsługi
SECTION 7 − SELECTING AND PREPARING A TUNGSTEN
FOR DC OR AC PHASE MACHINE WELDING
!
Whenever possible and practical, use DC weld output instead of AC weld output.
7-1. Selecting Tungsten Electrode (
A. Select Tungsten Electrode
.
Not all tungsten electrode manufacturers use the same colors to identify tungsten type. Contact the tungsten electrode manufacturer or refer-
ence the product packaging to identify the tungsten you are using.
Electrode Diameter
.040" (1 mm)
1/16" (1.6 mm)
3/32" (2.4 mm)
1/8" (3.2 mm)
.040" (1 mm)
1/16" (1.6 mm)
3/32" (2.4 mm)
1/8" (3.2 mm)
Typical argon shielding gas flow rates are 10 to 25 CFH (cubic feet per hour).
Figures listed are a guide and are a composite of recommendations from American Welding Society (AWS).

7-2. Preparing Tungsten Electrode For Welding With Phase Control Machines

!
Grinding the tungsten electrode produces dust and flying sparks which can cause injury and start fires. Use
local exhaust (forced ventilation) at the grinder or wear an approved respirator. Read MSDS for safety infor-
mation. Consider using tungsten containing ceria, lanthana, or yttria instead of thoria. Grinding dust from
thoriated electrodes contains low-level radioactive material. Properly dispose of grinder dust in an environ-
mentally safe way. Wear proper face, hand, and body protection. Keep flammables away.
A. Preparing Tungsten For DC Electrode Negative (DCEN) Welding
Radial Grinding
Causes Wandering Arc
Wrong Tungsten Preparation
B. Preparing Tungsten For AC Welding
OM-251981 Page 12
Wear Clean Gloves To Prevent Contamination Of Tungsten
Amperage Range - Gas Type
(DCEN) − Argon
Direct Current Electrode Negative
(For Use With Mild Or Stainless Steel)
2% Ceria Or 1.5% Lanthanum
15-80
70-150
150-250
250-400
Pure Tungsten
Pure Tungsten Not Recommended
For DCEN − Argon
1-1/2 To 4 Times
Electrode Diameter
2
4
Ideal Tungsten Preparation − Stable Arc
1 − 1-1/2 Times
Electrode Diameter
1
2
- Polarity
Unbalanced Wave
(For Use With Aluminum)
1
Grinding Wheel
Grind end of tungsten on fine grit, hard
abrasive wheel before welding. Do not use
wheel for other jobs or tungsten can become
contaminated causing lower weld quality.
2
Tungsten Electrode
3
A 2% ceriated tungsten is recommended.
15° to 30°
3
Ideal Grind Angle Range: 15° to 30°
.
30 degrees is the recommended elec-
trode grind angle.
1
4
Straight Ground
Grind lengthwise, not radial.
1
Tungsten Electrode
A pure tungsten is recommended..
2
Balled End
Ball end of tungsten by applying AC amper-
age recommended for a given electrode
diameter (see Section 7-1). Let ball on end of
the tungsten take its own shape.
Ref. gtaw_Phase_2018−01
)
AC − Argon
15-80
70-150
140-235
225-325
10-60
50-100
100-160
150-210